How do the AISI 51B60 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 51B60 (UNS G51601) side by side for 3 conditions: Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 51B60 material data sheets linked below.
AISI 51B60 Yield, Tensile and Hardness by Condition
| Condition | Yield strength (MPa) | Tensile strength (MPa) | Hardness (HV) | Elongation (%) |
|---|---|---|---|---|
| Oil Quenched & Tempered at 425°C | 1340–1640 | 1470–1800 | 415–505 | 9–13 |
| Oil Quenched & Tempered at 540°C | 990–1220 | 1080–1310 | 320–395 | 12–18 |
| Oil Quenched & Tempered at 650°C | 780–960 | 865–1070 | 265–325 | 16–24 |
AISI 51B60 Differences Compared with Oil Quenched & Tempered at 425°C
The table below shows how much each condition differs from the oil quenched & tempered at 425°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.
| Condition | Yield strength | Tensile strength | Hardness | Elongation |
|---|---|---|---|---|
| Oil Quenched & Tempered at 540°C | -26% | -27% | -22% | +36% |
| Oil Quenched & Tempered at 650°C | -42% | -41% | -36% | +82% |
AISI 51B60 Strength and Hardness Charts
AISI 51B60 Heat Treatment Key Points
The highest tensile strength is reached in the oil quenched & tempered at 425°C condition (1470–1800 MPa). The softest condition is oil quenched & tempered at 650°C (265–325 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 425°C to 650°C lowers hardness from 415–505 HV to 265–325 HV, trading strength for toughness and ductility.
AISI 51B60 Material Data Sheets
AISI 51B60 Oil Quenched & Tempered at 425°C | AISI 51B60 Oil Quenched & Tempered at 540°C | AISI 51B60 Oil Quenched & Tempered at 650°C | All AISI 51B60 conditions
Looking for AISI 51B60 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 51B60 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.