AISI 5160 Annealed vs Normalized vs Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 5160 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 5160 (UNS G51600) side by side for 7 conditions: Annealed, Normalized, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 5160 material data sheets linked below.

AISI 5160 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed245–305645–800183–22514–21
Normalized480–585860–1060248–30314–21
Oil Quenched & Tempered at 205°C1610–19802000–2450563–6933–5
Oil Quenched & Tempered at 315°C1590–19601800–2200500–6107–11
Oil Quenched & Tempered at 425°C1320–16101400–1810415–5058–12
Oil Quenched & Tempered at 540°C935–11501050–1290305–3759–15
Oil Quenched & Tempered at 650°C720–880805–990248–30316–24

AISI 5160 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+94%+33%+35%+0%
Oil Quenched & Tempered at 205°C+553%+208%+208%-77%
Oil Quenched & Tempered at 315°C+545%+177%+172%-49%
Oil Quenched & Tempered at 425°C+433%+122%+125%-43%
Oil Quenched & Tempered at 540°C+279%+62%+67%-31%
Oil Quenched & Tempered at 650°C+191%+24%+35%+14%

AISI 5160 Strength and Hardness Charts

AISI 5160 Yield strength (MPa)Annealed245–305Normalized480–585Q&T 205°C1610–1980Q&T 315°C1590–1960Q&T 425°C1320–1610Q&T 540°C935–1150Q&T 650°C720–880
AISI 5160 Tensile strength (MPa)Annealed645–800Normalized860–1060Q&T 205°C2000–2450Q&T 315°C1800–2200Q&T 425°C1400–1810Q&T 540°C1050–1290Q&T 650°C805–990
AISI 5160 Hardness (HV)Annealed183–225Normalized248–303Q&T 205°C563–693Q&T 315°C500–610Q&T 425°C415–505Q&T 540°C305–375Q&T 650°C248–303

AISI 5160 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (2000–2450 MPa). The softest condition is annealed (183–225 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 563–693 HV to 248–303 HV, trading strength for toughness and ductility.

AISI 5160 Material Data Sheets

AISI 5160 Annealed | AISI 5160 Normalized | AISI 5160 Oil Quenched & Tempered at 205°C | AISI 5160 Oil Quenched & Tempered at 315°C | AISI 5160 Oil Quenched & Tempered at 425°C | AISI 5160 Oil Quenched & Tempered at 540°C | AISI 5160 Oil Quenched & Tempered at 650°C | All AISI 5160 conditions

Looking for AISI 5160 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5160 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.