AISI 5150 Annealed vs Normalized vs Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 5150 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 5150 (UNS G51500) side by side for 7 conditions: Annealed, Normalized, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 5150 material data sheets linked below.

AISI 5150 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed320–395605–750160–23017–27
Normalized480–580780–960235–28517–25
Oil Quenched & Tempered at 205°C1560–19001750–2140470–5804–6
Oil Quenched & Tempered at 315°C1470–17501560–1920425–5254.5–7.5
Oil Quenched & Tempered at 425°C1280–14401300–1600370–4507–11
Oil Quenched & Tempered at 540°C925–11401010–1240310–38012–18
Oil Quenched & Tempered at 650°C725–890730–895248–30320–30

AISI 5150 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+48%+28%+33%-5%
Oil Quenched & Tempered at 205°C+384%+187%+169%-77%
Oil Quenched & Tempered at 315°C+350%+157%+144%-73%
Oil Quenched & Tempered at 425°C+280%+114%+110%-59%
Oil Quenched & Tempered at 540°C+189%+66%+77%-32%
Oil Quenched & Tempered at 650°C+126%+20%+41%+14%

AISI 5150 Strength and Hardness Charts

AISI 5150 Yield strength (MPa)Annealed320–395Normalized480–580Q&T 205°C1560–1900Q&T 315°C1470–1750Q&T 425°C1280–1440Q&T 540°C925–1140Q&T 650°C725–890
AISI 5150 Tensile strength (MPa)Annealed605–750Normalized780–960Q&T 205°C1750–2140Q&T 315°C1560–1920Q&T 425°C1300–1600Q&T 540°C1010–1240Q&T 650°C730–895
AISI 5150 Hardness (HV)Annealed160–230Normalized235–285Q&T 205°C470–580Q&T 315°C425–525Q&T 425°C370–450Q&T 540°C310–380Q&T 650°C248–303

AISI 5150 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1750–2140 MPa). The softest condition is annealed (160–230 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 470–580 HV to 248–303 HV, trading strength for toughness and ductility.

AISI 5150 Material Data Sheets

AISI 5150 Annealed | AISI 5150 Normalized | AISI 5150 Oil Quenched & Tempered at 205°C | AISI 5150 Oil Quenched & Tempered at 315°C | AISI 5150 Oil Quenched & Tempered at 425°C | AISI 5150 Oil Quenched & Tempered at 540°C | AISI 5150 Oil Quenched & Tempered at 650°C | All AISI 5150 conditions

Looking for AISI 5150 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5150 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.