AISI 5150 Normalized Material Data Sheet

AISI 5150 Normalized Material Data Sheet

AISI 5150 Normalized Overview

AISI 5150 normalized is AISI 5150 low alloy steel (UNS G51500) in the normalized condition. This AISI 5150 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 5150 conditions in our AISI 5150 yield, tensile and hardness comparison. Looking for AISI 5150 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5150 steel parts in-house and inspects them before shipment.

AISI 5150 Normalized Designation

AISI 5150
ConditionNormalized
UNS numberG51500
US nameSAE H51500, SAE 5150, SAE 5155, SAE 5150, ASTM 5150, ASTM G51500, ASTM 5155H, ASTM 5155, ASTM 5150H, ASTM 5150
JIS (Japanese) nameSUH11

AISI 5150 Normalized Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 5150 Normalized Composition detail

C (carbon)0.48–0.53%
Cr (chromium)0.7–0.9%
Fe (iron)97.2–98%
Mn (manganese)0.7–0.9%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 5150 Normalized Physical properties

Density7.8–7.9g/cm3

AISI 5150 Normalized Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)480–580MPa
Tensile strength780–960MPa
Specific strength61.1–73.9kN.m/kg
Elongation17–25% strain
Compressive strength480–580MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)480–580MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor45
Hardness – Vickers235–285HV
Elastic stored energy (springs)562–809kJ/m3
Fatigue strength at 10^7 cycles359–416MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
313–478MPa

AISI 5150 Normalized Impact & fracture properties

Fracture toughness75–118MPa.m0.5
Toughness (G)28.4–64.7kJ/m2

AISI 5150 Normalized Thermal properties

Melting point1410–1500°C
Maximum service temperature601–648°C
Minimum service temperature-68–-43°C
Thermal conductivity42–49W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient12–13.5µstrain/°C
Thermal shock resistance179–225°C
Thermal distortion resistance3.24–3.92MW/m
Latent heat of fusion265–280kJ/kg

AISI 5150 Normalized Electrical properties

Electrical resistivity21–28µohm.cm
Electrical conductivity6.16–8.21%IACS
Galvanic potential-0.5–-0.42V

AISI 5150 Normalized Magnetic properties

Magnetic typeMagnetic

AISI 5150 Normalized Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)5.6e-4–6.9e-4 

AISI 5150 Normalized Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed19.2 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Poor
Carbon equivalency0.737 – 0.86

AISI 5150 Normalized Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 5150 Normalized Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 5150 Normalized Standards with similar compositions

Australia: 5145 to AS 1444, 5145H to AS 1444, 5150 to AS 1444, 5155 to AS 1444, En11 to AS G18
Czech Republic: 422739 to CSN 422739
India: 50Cr4 to IS 1570/4, 50Cr4 to IS 2507, 50Cr4 to IS 3930, 55Cr3 to IS 13352, 55Cr3 to IS 1570/4, 55Cr70 to IS 1570
Mexico: 5145 to NMX-B-300, 5145H to NMX-B-268, 5145H to NMX-B-300, 5147 to NMX-B-300, 5147H to NMX-B-268, 5147H to NMX-B-300, 5150 to NMX-B-203-SCFI, 5150 to NMX-B-300, 5150H to NMX-B-268, 5150H to NMX-B-300, 5155 to NMX-B-300, 5155H to NMX-B-268, 5155H to NMX-B-300
Pan America: 5150 to COPANT 334
South Korea: SCr 445 to KS D 3707
Sweden: 2230 to SS 142230
USA: 5045, 5145, 5145 to ASTM A29/A29M, 5145 to ASTM A519, 5147, 5147 to ASTM A29/A29M, 5147 to ASTM A519, 5150 to ASTM A29/A29M, 5150 to ASTM A331-95, 5150 to ASTM A519, 5150 to ASTM A866, 5150 to SAE J404, 5150H to ASTM A331-95, 5152, 5155, 5155 to ASTM A29/A29M, 5155 to ASTM A331-95, 5155 to ASTM A519, 6150 to ASTM A331-95, G51500 to ASTM A1031, G51500 to ASTM A506, H51500 to SAE J775, NV6 to SAE J775, UNS G51450, UNS G51470, UNS G51500, UNS G51550, UNS H51450, UNS H51470, UNS H51500, UNS H51550
Tradenames: AIRCO 6150, POMPEY RMK, POMPEY TRK, VR-50, XK5150S, XK5155S