AISI 50B60 Tempering Temperature Comparison (315–650°C): Yield, Tensile & Hardness

How do the AISI 50B60 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 50B60 (UNS G50601) side by side for 4 conditions: Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 50B60 material data sheets linked below.

AISI 50B60 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 315°C1600–19501700–2070470–5756–10
Oil Quenched & Tempered at 425°C1240–15301360–1670390–4808–14
Oil Quenched & Tempered at 540°C900–11001010–1240315–38512–18
Oil Quenched & Tempered at 650°C700–860805–990260–32015–23

AISI 50B60 Differences Compared with Oil Quenched & Tempered at 315°C

The table below shows how much each condition differs from the oil quenched & tempered at 315°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 425°C-22%-20%-17%+38%
Oil Quenched & Tempered at 540°C-44%-40%-33%+88%
Oil Quenched & Tempered at 650°C-56%-52%-44%+138%

AISI 50B60 Strength and Hardness Charts

AISI 50B60 Yield strength (MPa)Q&T 315°C1600–1950Q&T 425°C1240–1530Q&T 540°C900–1100Q&T 650°C700–860
AISI 50B60 Tensile strength (MPa)Q&T 315°C1700–2070Q&T 425°C1360–1670Q&T 540°C1010–1240Q&T 650°C805–990
AISI 50B60 Hardness (HV)Q&T 315°C470–575Q&T 425°C390–480Q&T 540°C315–385Q&T 650°C260–320

AISI 50B60 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 315°C condition (1700–2070 MPa). The softest condition is oil quenched & tempered at 650°C (260–320 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 315°C to 650°C lowers hardness from 470–575 HV to 260–320 HV, trading strength for toughness and ductility.

AISI 50B60 Material Data Sheets