AISI 4340 Annealed vs Normalized vs Quenched & Tempered (205–650°C): Yield, Tensile & Hardness Compared

How do the AISI 4340 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 4340 (UNS G43400) side by side for 8 conditions: Annealed, Normalized, Quenched & Tempered, Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 4340 material data sheets linked below.

AISI 4340 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Annealed420–525670–820200–24517–27
Normalized770–9501150–1410325–4059–15
Quenched & Tempered1500–16501790–1980385–4758–10
Oil Quenched & Tempered at 205°C1510–18501580–2070465–5758–12
Oil Quenched & Tempered at 315°C1430–17501550–1990435–5358–12
Oil Quenched & Tempered at 425°C1230–15001320–1620385–4758–12
Oil Quenched & Tempered at 540°C965–11901050–1300325–40010–16
Oil Quenched & Tempered at 650°C770–940865–1070255–31515–23

AISI 4340 Differences Compared with Annealed

The table below shows how much each condition differs from the annealed condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Normalized+82%+72%+64%-45%
Quenched & Tempered+233%+153%+93%-59%
Oil Quenched & Tempered at 205°C+256%+145%+134%-55%
Oil Quenched & Tempered at 315°C+237%+138%+118%-55%
Oil Quenched & Tempered at 425°C+189%+97%+93%-55%
Oil Quenched & Tempered at 540°C+128%+58%+63%-41%
Oil Quenched & Tempered at 650°C+81%+30%+28%-14%

AISI 4340 Strength and Hardness Charts

AISI 4340 Yield strength (MPa)Annealed420–525Normalized770–950Q&T1500–1650Q&T 205°C1510–1850Q&T 315°C1430–1750Q&T 425°C1230–1500Q&T 540°C965–1190Q&T 650°C770–940
AISI 4340 Tensile strength (MPa)Annealed670–820Normalized1150–1410Q&T1790–1980Q&T 205°C1580–2070Q&T 315°C1550–1990Q&T 425°C1320–1620Q&T 540°C1050–1300Q&T 650°C865–1070
AISI 4340 Hardness (HV)Annealed200–245Normalized325–405Q&T385–475Q&T 205°C465–575Q&T 315°C435–535Q&T 425°C385–475Q&T 540°C325–400Q&T 650°C255–315

AISI 4340 Heat Treatment Key Points

The highest tensile strength is reached in the quenched & tempered condition (1790–1980 MPa). The softest condition is annealed (200–245 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 465–575 HV to 255–315 HV, trading strength for toughness and ductility.

AISI 4340 Material Data Sheets

AISI 4340 Annealed | AISI 4340 Normalized | AISI 4340 Quenched & Tempered | AISI 4340 Oil Quenched & Tempered at 205°C | AISI 4340 Oil Quenched & Tempered at 315°C | AISI 4340 Oil Quenched & Tempered at 425°C | AISI 4340 Oil Quenched & Tempered at 540°C | AISI 4340 Oil Quenched & Tempered at 650°C | All AISI 4340 conditions