D6AC quenched tempered is D6AC low alloy steel (UNS K24728) in the quenched & tempered condition. This D6AC quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for D6AC parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined D6AC steel parts in-house and inspects them before shipment.
D6AC Quenched & Tempered Designation
D6AC
Condition
Quenched & tempered
UNS number
K24728
US name
AMS 6431, ASTM A646 Grade 9, ASTM A579 Grade 23
D6AC Quenched & Tempered Typical uses
General construction, general mechanical engineering, automotive, pressure vessels, pipework
D6AC Quenched & Tempered Composition detail
C (carbon)
0.45
–
0.5
%
Cr (chromium)
0.9
–
1.2
%
Fe (iron)
95.1
–
96.5
%
Mn (manganese)
0.6
–
0.9
%
Mo (molybdenum)
0.9
–
1.1
%
Ni (nickel)
0.4
–
0.7
%
P (phosphorus)
0
–
0.01
%
S (sulfur)
0
–
0.01
%
Si (silicon)
0.15
–
0.3
%
V (vanadium)
0.08
–
0.15
%
D6AC Quenched & Tempered Physical properties
Density
7.79
–
7.87
g/cm3
D6AC Quenched & Tempered Mechanical properties
Young’s modulus
200
–
210
GPa
Specific stiffness
25.5
–
26.9
MN.m/kg
Yield strength (elastic limit)
1310
–
1450
MPa
Tensile strength
1520
–
1680
MPa
Specific strength
167
–
185
kN.m/kg
Elongation
7
–
12
% strain
Compressive strength
1370
–
1510
MPa
Flexural modulus
200
–
210
GPa
Flexural strength (modulus of rupture)
1310
–
1450
MPa
Shear modulus
76
–
79.9
GPa
Bulk modulus
185
–
195
GPa
Poisson’s ratio
0.32
–
0.333
Shape factor
17
Hardness – Vickers
400
–
500
HV
Hardness – Rockwell C
45
–
47
HRC
Elastic stored energy (springs)
4180
–
5110
kJ/m3
Fatigue strength at 10^7 cycles
683
–
835
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles