AISI 8735 Normalized Material Data Sheet

AISI 8735 Normalized Material Data Sheet

AISI 8735 Normalized Overview

AISI 8735 normalized is AISI 8735 low alloy steel (UNS G87350) in the normalized condition. This AISI 8735 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for AISI 8735 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8735 steel parts in-house and inspects them before shipment.

AISI 8735 Normalized Designation

AISI 8735
ConditionNormalized
UNS numberG87350
US name~ASTM G87350

AISI 8735 Normalized Typical uses

General construction, general mechanical engineering, automotive, pressure vessels, pipework

AISI 8735 Normalized Composition detail

C (carbon)0.33–0.38%
Cr (chromium)0.4–0.6%
Fe (iron)96.6–97.8%
Mn (manganese)0.75–1%
Mo (molybdenum)0.2–0.3%
Ni (nickel)0.4–0.7%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 8735 Normalized Physical properties

Density7.79–7.87g/cm3

AISI 8735 Normalized Mechanical properties

Young’s modulus200–210GPa
Specific stiffness25.5–26.9MN.m/kg
Yield strength (elastic limit)483–534MPa
Tensile strength621–686MPa
Specific strength61.6–68.2kN.m/kg
Elongation8–18% strain
Compressive strength483–534MPa
Flexural modulus200–210GPa
Flexural strength (modulus of rupture)483–534MPa
Shear modulus76–79.9GPa
Bulk modulus185–195GPa
Poisson’s ratio0.32–0.333 
Shape factor46
Hardness – Vickers167–500HV
Elastic stored energy (springs)569–695kJ/m3
Fatigue strength at 10^7 cycles280–295MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
256–323MPa

AISI 8735 Normalized Impact & fracture properties

Fracture toughness90–110MPa.m0.5
Toughness (G)39.8–58.5kJ/m2

AISI 8735 Normalized Thermal properties

Melting point1260–1580°C
Maximum service temperature445–496°C
Minimum service temperature-73–-48°C
Thermal conductivity55–59.6W/m.°C
Specific heat capacity461–480J/kg.°C
Thermal expansion coefficient12.4–13.1µstrain/°C
Thermal shock resistance183–207°C
Thermal distortion resistance4.29–4.71MW/m
Latent heat of fusion283–326kJ/kg

AISI 8735 Normalized Electrical properties

Electrical resistivity13–46µohm.cm
Electrical conductivity3.75–13.3%IACS
Galvanic potential-0.51–-0.43V

AISI 8735 Normalized Magnetic properties

Magnetic typeMagnetic

AISI 8735 Normalized Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5050–5180m/s
Mechanical loss coefficient (tan delta)5e-4–7e-4 

AISI 8735 Normalized Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed19.5 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.602 – 0.773

AISI 8735 Normalized Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 8735 Normalized Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 8735 Normalized Notes

AISI 8735 Normalized Warning
Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C

AISI 8735 Normalized Standards with similar compositions

Mexico: 8637 to NMX-B-300, 8637H to NMX-B-268, 8637H to NMX-B-300
Pan America: 8637 to COPANT 514
USA: 6282 to AMS 6282G, 8635, 8637, 8637 to ASTM A29/A29M, 8637 to ASTM A322-91, 8637 to ASTM A331-95, 8637 to ASTM A752/A752M, 8637 to ASTM A829/A829M, 8637 to SAE J404, 8637H, 8637H to ASTM A304, 8637H to SAE J1268, 8735, 8735 to ASTM A519, G87350 to ASTM A1031, UNS G86370, UNS G87350, UNS H86370