Home » Low Alloy Steel Grades » 4335V Low Alloy Steel » 4335V Quenched & Tempered Material Data Sheet
4335V Quenched & Tempered Material Data Sheet
4335V Quenched & Tempered Overview
4335V quenched tempered is 4335V low alloy steel (UNS K33517, EN 38NiCrMoV7-3) in the quenched & tempered condition. This 4335V quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 4335V parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 4335V steel parts in-house and inspects them before shipment.
4335V Quenched & Tempered Designation
4335V Condition Quenched & tempered UNS number K33517, K23477 US name AMS 6433, AMS 6435, ASTM A646 Grade 6, ASTM A579 Grade 21 EN name 38NiCrMoV7-3 EN number 1.6926, 1.6944
4335V Quenched & Tempered Typical uses
General construction, general mechanical engineering, automotive, pressure vessels, pipework
4335V Quenched & Tempered Composition detail
C (carbon) 0.32 – 0.38 % Cr (chromium) 0.65 – 0.9 % Fe (iron) 94.6 – 96.1 % Mn (manganese) 0.6 – 0.9 % Mo (molybdenum) 0.3 – 0.4 % Ni (nickel) 1.65 – 2 % S (sulfur) 0 – 0.04 % Si (silicon) 0.2 – 0.6 % V (vanadium) 0.17 – 0.23 %
4335V Quenched & Tempered Physical properties
4335V Quenched & Tempered Mechanical properties
Young’s modulus 200 – 210 GPa Specific stiffness 25.5 – 26.9 MN.m/kg Yield strength (elastic limit) 1310 – 1450 MPa Tensile strength 1410 – 1660 MPa Specific strength 167 – 185 kN.m/kg Elongation 7 – 10 % strain Compressive strength 1370 – 1520 MPa Flexural modulus 200 – 210 GPa Flexural strength (modulus of rupture) 1310 – 1450 MPa Shear modulus 76 – 79.9 GPa Bulk modulus 185 – 195 GPa Poisson’s ratio 0.32 – 0.333 Shape factor 17 Hardness – Vickers 490 – 590 HV Hardness – Brinell 450 – 550 HB Elastic stored energy (springs) 4180 – 5110 kJ/m3 Fatigue strength at 10^7 cycles 515 – 555 MPa Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles 457 – 626 MPa
4335V Quenched & Tempered Impact & fracture properties
Fracture toughness 92 – 115 MPa.m0.5 Toughness (G) 41.7 – 63.8 kJ/m2
4335V Quenched & Tempered Thermal properties
Melting point 1260 – 1580 °C Maximum service temperature 232 – 260 °C Minimum service temperature -73 – -43 °C Thermal conductivity 50 – 54.2 W/m.°C Specific heat capacity 461 – 480 J/kg.°C Thermal expansion coefficient 12.4 – 13.1 µstrain/°C Thermal shock resistance 496 – 560 °C Thermal distortion resistance 3.9 – 4.28 MW/m Latent heat of fusion 284 – 326 kJ/kg
4335V Quenched & Tempered Electrical properties
Electrical resistivity 14 – 46 µohm.cm Electrical conductivity 3.75 – 12.3 %IACS Galvanic potential -0.5 – -0.42 V
4335V Quenched & Tempered Magnetic properties
4335V Quenched & Tempered Optical, aesthetic and acoustic properties
Transparency Opaque Acoustic velocity 5050 – 5180 m/s Mechanical loss coefficient (tan delta) 2e-4 – 5e-4
4335V Quenched & Tempered Processing properties
Metal casting Unsuitable Metal cold forming Excellent Metal hot forming Excellent Metal press forming Excellent Metal deep drawing Limited use Machining speed 8.84 m/min Weldability Notes: Preheating and post weld heat treatments may be required Good Carbon equivalency 0.754 – 0.969
4335V Quenched & Tempered Durability
Water (fresh) Acceptable Water (salt) Limited use Weak acids Limited use Strong acids Unacceptable Weak alkalis Acceptable Strong alkalis Limited use Organic solvents Excellent Oxidation at 500C Acceptable UV radiation (sunlight) Excellent Galling resistance (adhesive wear) Acceptable Flammability Non-flammable
4335V Quenched & Tempered Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments Susceptible
4335V Quenched & Tempered Notes
4335V Quenched & Tempered Warning Some rare heat treatments of certain alloys may produce values for mechanical properties outside the given ranges, e.g. AISI 9255. tempered at 205C
4335V Quenched & Tempered Standards with similar compositions
USA: 21 to ASTM A579, 22 to ASTM A579, 6435 to AMS 6435, B24V to ASTM A540/A540M, Grade 6 to ASTM A646-95, UNS K23477, UNS K24070, UNS K33517Tradenames: KRUPP HFX 6926, KRUPP WL 1.6944, LESCALLOY 4335 +V VAC-ARC, SV-RHF 10, WITTEN CNOV 37 L VA
4335V Low Alloy Steel
4335V Material Data Sheets
Q&T Quenched & Tempered You are here
All 4335V Conditions
Modulus Metal Services
Manufacturing & Quality Services in Turkey