4330V quenched tempered is 4330V low alloy steel (UNS K23080, EN 38NiCrMoV7-3) in the quenched & tempered condition. This 4330V quenched tempered material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Looking for 4330V parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined 4330V steel parts in-house and inspects them before shipment.
4330V Quenched & Tempered Designation
4330V
Condition
Quenched & tempered
UNS number
K23080
US name
AMS 6411, AMS 6427, AMS 6428, ASTM A646 Grade 5
EN name
G32NiCrMo8-5-4, 38NiCrMoV7-3
EN number
1.6570, 1.6926
4330V Quenched & Tempered Typical uses
General construction, general mechanical engineering, automotive, pressure vessels, pipework
4330V Quenched & Tempered Composition detail
C (carbon)
0.28
–
0.33
%
Cr (chromium)
0.75
–
1
%
Cu (copper)
0
–
0.35
%
Fe (iron)
94.4
–
96.1
%
Mn (manganese)
0.65
–
1
%
Mo (molybdenum)
0.35
–
0.5
%
Ni (nickel)
1.65
–
2
%
Si (silicon)
0.15
–
0.35
%
V (vanadium)
0.05
–
0.1
%
4330V Quenched & Tempered Physical properties
Density
7.79
–
7.87
g/cm3
4330V Quenched & Tempered Mechanical properties
Young’s modulus
200
–
210
GPa
Specific stiffness
25.5
–
26.9
MN.m/kg
Yield strength (elastic limit)
1280
–
1410
MPa
Tensile strength
1520
–
1680
MPa
Specific strength
163
–
180
kN.m/kg
Elongation
5
–
10
% strain
Compressive strength
1330
–
1470
MPa
Flexural modulus
200
–
210
GPa
Flexural strength (modulus of rupture)
1280
–
1410
MPa
Shear modulus
76
–
79.9
GPa
Bulk modulus
185
–
195
GPa
Poisson’s ratio
0.32
–
0.333
Shape factor
17
Hardness – Vickers
490
–
590
HV
Hardness – Brinell
450
–
550
HB
Elastic stored energy (springs)
3970
–
4850
kJ/m3
Fatigue strength at 10^7 cycles
606
–
682
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles