AISI 94B30 Oil Quenched & Tempered at 315°C Material Data Sheet
AISI 94B30 Oil Quenched & Tempered at 315°C Material Data Sheet
AISI 94B30 Oil Quenched & Tempered at 315°C Overview
AISI 94B30 tempered 315°C is AISI 94B30 low alloy steel (UNS G94301) in the oil quenched & tempered at 315°C condition. This AISI 94B30 tempered 315°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 94B30 conditions in our AISI 94B30 yield, tensile and hardness comparison. Looking for AISI 94B30 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 94B30 steel parts in-house and inspects them before shipment.
AISI 94B30 Oil Quenched & Tempered at 315°C Designation
AISI 94B30
Condition
Tempered at 315°C & oil quenched
UNS number
G94301
AISI 94B30 Oil Quenched & Tempered at 315°C Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 94B30 Oil Quenched & Tempered at 315°C Composition detail
B (boron)
5e-4
–
0.003
%
C (carbon)
0.28
–
0.33
%
Cr (chromium)
0.3
–
0.5
%
Fe (iron)
97
–
98.1
%
Mn (manganese)
0.75
–
1
%
Mo (molybdenum)
0.08
–
0.15
%
Ni (nickel)
0.3
–
0.6
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 94B30 Oil Quenched & Tempered at 315°C Physical properties
Density
7.8
–
7.9
g/cm3
AISI 94B30 Oil Quenched & Tempered at 315°C Mechanical properties
Young’s modulus
206
–
216
GPa
Specific stiffness
26.2
–
27.5
MN.m/kg
Yield strength (elastic limit)
1280
–
1570
MPa
Tensile strength
1440
–
1760
MPa
Specific strength
162
–
199
kN.m/kg
Elongation
9
–
15
% strain
Compressive strength
1270
–
1570
MPa
Flexural modulus
206
–
216
GPa
Flexural strength (modulus of rupture)
1280
–
1570
MPa
Shear modulus
79
–
85
GPa
Bulk modulus
159
–
176
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
17
Hardness – Vickers
400
–
490
HV
Elastic stored energy (springs)
3890
–
5760
kJ/m3
Fatigue strength at 10^7 cycles
552
–
636
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
AISI 94B30 Oil Quenched & Tempered at 315°C Thermal properties
Melting point
1460
–
1510
°C
Maximum service temperature
275
–
305
°C
Minimum service temperature
-53
–
-28
°C
Thermal conductivity
46
–
51
W/m.°C
Specific heat capacity
425
–
475
J/kg.°C
Thermal expansion coefficient
11
–
13
µstrain/°C
Thermal shock resistance
491
–
639
°C
Thermal distortion resistance
3.68
–
4.46
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 94B30 Oil Quenched & Tempered at 315°C Electrical properties
Electrical resistivity
15
–
35
µohm.cm
Electrical conductivity
4.93
–
11.5
%IACS
Galvanic potential
-0.51
–
-0.43
V
AISI 94B30 Oil Quenched & Tempered at 315°C Magnetic properties
Magnetic type
Magnetic
AISI 94B30 Oil Quenched & Tempered at 315°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5120
–
5250
m/s
Mechanical loss coefficient (tan delta)
2.5e-4
–
3.1e-4
AISI 94B30 Oil Quenched & Tempered at 315°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
10.4 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.501 – 0.667
AISI 94B30 Oil Quenched & Tempered at 315°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 94B30 Oil Quenched & Tempered at 315°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible
AISI 94B30 Oil Quenched & Tempered at 315°C Standards with similar compositions
Mexico: 94B30 to NMX-B-203-SCFI, 94B30 to NMX-B-300, 94B30H to NMX-B-268, 94B30H to NMX-B-300
Pan America: 94B30 to COPANT 514
USA: 94B30, 94B30 to ASTM A29/A29M, 94B30 to ASTM A322-91, 94B30 to ASTM A331-95, 94B30 to ASTM A519, 94B30 to ASTM A752/A752M, 94B30 to SAE J770, 94B30H, 94B30H to ASTM A304, 94B30H to ASTM A331-95, 94B30H to SAE J1268, EX 47, EX 48, EX 49, EX 50, UNS G94301, UNS H94301, UNS K13521