AISI 9260 Oil Quenched & Tempered at 650°C Material Data Sheet
AISI 9260 Oil Quenched & Tempered at 650°C Overview
| AISI 9260 tempered 650°C is AISI 9260 low alloy steel (UNS G92600, EN 60Si7) in the oil quenched & tempered at 650°C condition. This AISI 9260 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 9260 conditions in our AISI 9260 yield, tensile and hardness comparison. Looking for AISI 9260 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 9260 steel parts in-house and inspects them before shipment. |
AISI 9260 Oil Quenched & Tempered at 650°C Designation
| AISI 9260 | |
| Condition | Tempered at 650°C & oil quenched |
| UNS number | G92600 |
| EN name | EN45A, 250A61, 250A58, 60Si7 |
| EN number | 1.5028 |
AISI 9260 Oil Quenched & Tempered at 650°C Typical uses
| Laminated springs, coil springs, torsion bars of heavy section |
AISI 9260 Oil Quenched & Tempered at 650°C Composition detail
| C (carbon) | 0.55 | – | 0.65 | % |
| Fe (iron) | 96.1 | – | 96.9 | % |
| Mn (manganese) | 0.75 | – | 1 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 1.8 | – | 2.2 | % |
AISI 9260 Oil Quenched & Tempered at 650°C Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 9260 Oil Quenched & Tempered at 650°C Mechanical properties
| Young’s modulus | 203 | – | 211 | GPa |
| Specific stiffness | 25.8 | – | 26.9 | MN.m/kg |
| Yield strength (elastic limit) | 730 | – | 895 | MPa |
| Tensile strength | 880 | – | 1080 | MPa |
| Specific strength | 93 | – | 114 | kN.m/kg |
| Elongation | 16 | – | 24 | % strain |
| Compressive strength | 730 | – | 895 | MPa |
| Flexural modulus | 203 | – | 211 | GPa |
| Flexural strength (modulus of rupture) | 730 | – | 895 | MPa |
| Shear modulus | 78 | – | 83 | GPa |
| Bulk modulus | 157 | – | 172 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 30 | |||
| Hardness – Vickers | 270 | – | 330 | HV |
| Elastic stored energy (springs) | 1300 | – | 1920 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 391 | – | 452 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 341 | – | 519 | MPa |
AISI 9260 Oil Quenched & Tempered at 650°C Impact & fracture properties
| Fracture toughness | 48 | – | 79 | MPa.m0.5 |
| Toughness (G) | 11.7 | – | 28.7 | kJ/m2 |
AISI 9260 Oil Quenched & Tempered at 650°C Thermal properties
| Melting point | 1380 | – | 1490 | °C |
| Maximum service temperature | 587 | – | 640 | °C |
| Minimum service temperature | -68 | – | -38 | °C |
| Thermal conductivity | 46 | – | 51 | W/m.°C |
| Specific heat capacity | 425 | – | 475 | J/kg.°C |
| Thermal expansion coefficient | 11 | – | 13 | µstrain/°C |
| Thermal shock resistance | 287 | – | 372 | °C |
| Thermal distortion resistance | 3.68 | – | 4.46 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 9260 Oil Quenched & Tempered at 650°C Electrical properties
| Electrical resistivity | 15 | – | 35 | µohm.cm |
| Electrical conductivity | 4.93 | – | 11.5 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 9260 Oil Quenched & Tempered at 650°C Magnetic properties
| Magnetic type | Magnetic |
AISI 9260 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5080 | – | 5190 | m/s |
| Mechanical loss coefficient (tan delta) | 4.2e-4 | – | 5.3e-4 | |
AISI 9260 Oil Quenched & Tempered at 650°C Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 16.5 m/min |
| Weldability Notes: Preheating and post weld heat treatments may be required | Poor |
| Carbon equivalency | 0.675 – 0.817 |
AISI 9260 Oil Quenched & Tempered at 650°C Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 9260 Oil Quenched & Tempered at 650°C Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Slightly susceptible |
AISI 9260 Oil Quenched & Tempered at 650°C Notes
| AISI 9260 Oil Quenched & Tempered at 650°C Other notes |
| A spring steel, used for more highly stressed applications than carbon steels. |
AISI 9260 Oil Quenched & Tempered at 650°C Standards with similar compositions
| Argentina: IRAM 9260 to IAS |
| Australia: 9260 to AS 1444, 9260H to AS 1444 |
| Belgium: 60Si7 to NBN 253-05 |
| France: 60S7 to AFNOR, 760S7 to AFNOR |
| Germany: 1.0909 to DIN |
| Hungary: 60S to MSZ 4217, 61Si7 to MSZ 2666 |
| India: 55Si7 to IS 3431, 60Si7 to IS 1570/4, 60Si7 to IS 3195, 60Si7 to IS 3431, 60Si7 to IS 4072, 60Si7 to IS 8052, 60Si7 to IS 8055, 65Si7 to IS 1570/4, 65Si7 to IS 3431, 65Si7 to IS 8052, Grade 3 to IS 8051, Grade 4 to IS 8051 |
| International: 60Si8 to ISO 683-14 |
| Italy: 60Si7 to UNI 3545 |
| Japan: SUP 7 to JIS G4801 |
| Mexico: 9260 to NMX-B-203-SCFI, 9260 to NMX-B-300, 9260H to NMX-B-268, 9260H to NMX-B-300 |
| Pan America: 9260 to COPANT 334 |
| South Korea: SPS 3 to KS D 3701, SPS 4 to KS D 3701 |
| Spain: 60Si7 to UNE 36015, F.1441 to UNE 36015 |
| UK: 250A58 to BS 970/1, 250A58 to BS 970/5, 250A61 to BS 970/1 |
| USA: 9260 to ASTM A29/A29M, 9260 to ASTM A331-95, 9260 to ASTM A519, 9260 to SAE J404, G92600 to ASTM A1031, UNS G92600, UNS H92600 |
| Tradenames: 60 SI 7, AMBO MS 6, BOHLER F105, BOHLER F108, DAWSON, FLEXO STEEL, FRANXA 9, HECLA S55, KRUPP 60 SI 7, KRUPP 65 SI 7, LA BELLE 2-70, MACCO SILICON MANGANESE, MS5E, MULTOLE, OVAKO 571, POMPEY RS 4, POMPEY RS4E, R-P, SILEX-65, SILICO MANGANESE SPRING, SISCO OIL HARDENING CHISEL, S-M, SODERFORS NO. 43, U.S.S. 9260, VS-60, XK9258S |