AISI 9260 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 9260 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 9260 Oil Quenched & Tempered at 425°C Overview

AISI 9260 tempered 425°C is AISI 9260 low alloy steel (UNS G92600, EN 60Si7) in the oil quenched & tempered at 425°C condition. This AISI 9260 tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 9260 conditions in our AISI 9260 yield, tensile and hardness comparison. Looking for AISI 9260 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 9260 steel parts in-house and inspects them before shipment.

AISI 9260 Oil Quenched & Tempered at 425°C Designation

AISI 9260
ConditionTempered at 425°C & oil quenched
UNS numberG92600
EN nameEN45A, 250A61, 250A58, 60Si7
EN number1.5028

AISI 9260 Oil Quenched & Tempered at 425°C Typical uses

Laminated springs, coil springs, torsion bars of heavy section

AISI 9260 Oil Quenched & Tempered at 425°C Composition detail

C (carbon)0.55–0.65%
Fe (iron)96.1–96.9%
Mn (manganese)0.75–1%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)1.8–2.2%

AISI 9260 Oil Quenched & Tempered at 425°C Physical properties

Density7.8–7.9g/cm3

AISI 9260 Oil Quenched & Tempered at 425°C Mechanical properties

Young’s modulus203–211GPa
Specific stiffness25.8–26.9MN.m/kg
Yield strength (elastic limit)1350–1660MPa
Tensile strength1580–1940MPa
Specific strength172–211kN.m/kg
Elongation6–10% strain
Compressive strength1350–1660MPa
Flexural modulus203–211GPa
Flexural strength (modulus of rupture)1350–1660MPa
Shear modulus78–83GPa
Bulk modulus157–172GPa
Poisson’s ratio0.285–0.295 
Shape factor15
Hardness – Vickers420–520HV
Elastic stored energy (springs)4440–6560kJ/m3
Fatigue strength at 10^7 cycles589–681MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
515–779MPa

AISI 9260 Oil Quenched & Tempered at 425°C Impact & fracture properties

Fracture toughness29–56MPa.m0.5
Toughness (G)4.41–14kJ/m2

AISI 9260 Oil Quenched & Tempered at 425°C Thermal properties

Melting point1380–1490°C
Maximum service temperature385–415°C
Minimum service temperature-53–-23°C
Thermal conductivity46–51W/m.°C
Specific heat capacity425–475J/kg.°C
Thermal expansion coefficient11–13µstrain/°C
Thermal shock resistance530–688°C
Thermal distortion resistance3.68–4.46MW/m
Latent heat of fusion265–280kJ/kg

AISI 9260 Oil Quenched & Tempered at 425°C Electrical properties

Electrical resistivity15–35µohm.cm
Electrical conductivity4.93–11.5%IACS
Galvanic potential-0.51–-0.43V

AISI 9260 Oil Quenched & Tempered at 425°C Magnetic properties

Magnetic typeMagnetic

AISI 9260 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5080–5190m/s
Mechanical loss coefficient (tan delta)2.3e-4–2.9e-4 

AISI 9260 Oil Quenched & Tempered at 425°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed9.75 m/min
Weldability
Notes: Preheating and post weld heat treatments may be required
Poor
Carbon equivalency0.675 – 0.817

AISI 9260 Oil Quenched & Tempered at 425°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 9260 Oil Quenched & Tempered at 425°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible

AISI 9260 Oil Quenched & Tempered at 425°C Notes

AISI 9260 Oil Quenched & Tempered at 425°C Other notes
A spring steel, used for more highly stressed applications than carbon steels.

AISI 9260 Oil Quenched & Tempered at 425°C Standards with similar compositions

Argentina: IRAM 9260 to IAS
Australia: 9260 to AS 1444, 9260H to AS 1444
Belgium: 60Si7 to NBN 253-05
France: 60S7 to AFNOR, 760S7 to AFNOR
Germany: 1.0909 to DIN
Hungary: 60S to MSZ 4217, 61Si7 to MSZ 2666
India: 55Si7 to IS 3431, 60Si7 to IS 1570/4, 60Si7 to IS 3195, 60Si7 to IS 3431, 60Si7 to IS 4072, 60Si7 to IS 8052, 60Si7 to IS 8055, 65Si7 to IS 1570/4, 65Si7 to IS 3431, 65Si7 to IS 8052, Grade 3 to IS 8051, Grade 4 to IS 8051
International: 60Si8 to ISO 683-14
Italy: 60Si7 to UNI 3545
Japan: SUP 7 to JIS G4801
Mexico: 9260 to NMX-B-203-SCFI, 9260 to NMX-B-300, 9260H to NMX-B-268, 9260H to NMX-B-300
Pan America: 9260 to COPANT 334
South Korea: SPS 3 to KS D 3701, SPS 4 to KS D 3701
Spain: 60Si7 to UNE 36015, F.1441 to UNE 36015
UK: 250A58 to BS 970/1, 250A58 to BS 970/5, 250A61 to BS 970/1
USA: 9260 to ASTM A29/A29M, 9260 to ASTM A331-95, 9260 to ASTM A519, 9260 to SAE J404, G92600 to ASTM A1031, UNS G92600, UNS H92600
Tradenames: 60 SI 7, AMBO MS 6, BOHLER F105, BOHLER F108, DAWSON, FLEXO STEEL, FRANXA 9, HECLA S55, KRUPP 60 SI 7, KRUPP 65 SI 7, LA BELLE 2-70, MACCO SILICON MANGANESE, MS5E, MULTOLE, OVAKO 571, POMPEY RS 4, POMPEY RS4E, R-P, SILEX-65, SILICO MANGANESE SPRING, SISCO OIL HARDENING CHISEL, S-M, SODERFORS NO. 43, U.S.S. 9260, VS-60, XK9258S