AISI 86B45 Oil Quenched & Tempered at 540°C Material Data Sheet
AISI 86B45 Oil Quenched & Tempered at 540°C Material Data Sheet
AISI 86B45 Oil Quenched & Tempered at 540°C Overview
AISI 86B45 tempered 540°C is AISI 86B45 low alloy steel (UNS G86451) in the oil quenched & tempered at 540°C condition. This AISI 86B45 tempered 540°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 86B45 conditions in our AISI 86B45 yield, tensile and hardness comparison. Looking for AISI 86B45 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 86B45 steel parts in-house and inspects them before shipment.
AISI 86B45 Oil Quenched & Tempered at 540°C Designation
AISI 86B45
Condition
Tempered at 540°C & oil quenched
UNS number
G86451
AISI 86B45 Oil Quenched & Tempered at 540°C Typical uses
General construction, general mechanical engineering, automotive, tools, axles, gears, springs.
AISI 86B45 Oil Quenched & Tempered at 540°C Composition detail
B (boron)
5e-4
–
0.003
%
C (carbon)
0.43
–
0.48
%
Cr (chromium)
0.4
–
0.6
%
Fe (iron)
96.5
–
97.7
%
Mn (manganese)
0.75
–
1
%
Mo (molybdenum)
0.15
–
0.25
%
Ni (nickel)
0.4
–
0.7
%
P (phosphorus)
0
–
0.035
%
S (sulfur)
0
–
0.04
%
Si (silicon)
0.15
–
0.35
%
AISI 86B45 Oil Quenched & Tempered at 540°C Physical properties
Density
7.8
–
7.9
g/cm3
AISI 86B45 Oil Quenched & Tempered at 540°C Mechanical properties
Young’s modulus
201
–
212
GPa
Specific stiffness
25.6
–
27
MN.m/kg
Yield strength (elastic limit)
925
–
1140
MPa
Tensile strength
990
–
1220
MPa
Specific strength
118
–
145
kN.m/kg
Elongation
12
–
18
% strain
Compressive strength
925
–
1140
MPa
Flexural modulus
201
–
212
GPa
Flexural strength (modulus of rupture)
925
–
1140
MPa
Shear modulus
77
–
83
GPa
Bulk modulus
155
–
173
GPa
Poisson’s ratio
0.285
–
0.295
Shape factor
23
Hardness – Vickers
303
–
373
HV
Elastic stored energy (springs)
2090
–
3120
kJ/m3
Fatigue strength at 10^7 cycles
425
–
491
MPa
Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
AISI 86B45 Oil Quenched & Tempered at 540°C Thermal properties
Melting point
1420
–
1500
°C
Maximum service temperature
500
–
530
°C
Minimum service temperature
-63
–
-38
°C
Thermal conductivity
35
–
46
W/m.°C
Specific heat capacity
460
–
500
J/kg.°C
Thermal expansion coefficient
11
–
12.5
µstrain/°C
Thermal shock resistance
375
–
480
°C
Thermal distortion resistance
2.95
–
3.97
MW/m
Latent heat of fusion
265
–
280
kJ/kg
AISI 86B45 Oil Quenched & Tempered at 540°C Electrical properties
Electrical resistivity
23
–
35
µohm.cm
Electrical conductivity
4.93
–
7.5
%IACS
Galvanic potential
-0.5
–
-0.42
V
AISI 86B45 Oil Quenched & Tempered at 540°C Magnetic properties
Magnetic type
Magnetic
AISI 86B45 Oil Quenched & Tempered at 540°C Optical, aesthetic and acoustic properties
Transparency
Opaque
Acoustic velocity
5060
–
5200
m/s
Mechanical loss coefficient (tan delta)
3.5e-4
–
4.4e-4
AISI 86B45 Oil Quenched & Tempered at 540°C Processing properties
Metal casting
Unsuitable
Metal cold forming
Excellent
Metal hot forming
Excellent
Metal press forming
Excellent
Metal deep drawing
Limited use
Machining speed
14 m/min
Weldability Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency
0.692 – 0.863
AISI 86B45 Oil Quenched & Tempered at 540°C Durability
Water (fresh)
Acceptable
Water (salt)
Limited use
Weak acids
Limited use
Strong acids
Unacceptable
Weak alkalis
Acceptable
Strong alkalis
Limited use
Organic solvents
Excellent
Oxidation at 500C
Acceptable
UV radiation (sunlight)
Excellent
Galling resistance (adhesive wear)
Acceptable
Flammability
Non-flammable
AISI 86B45 Oil Quenched & Tempered at 540°C Corrosion resistance
Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible
AISI 86B45 Oil Quenched & Tempered at 540°C Standards with similar compositions
Australia: 8645 to AS 1444, 8645H to AS 1444
Mexico: 8645 to NMX-B-203-SCFI, 8645 to NMX-B-300, 8645H to NMX-B-268, 8645H to NMX-B-300, 86B45H to NMX-B-268, 86B45H to NMX-B-300
Pan America: 8645 to COPANT 514, 86B45 to COPANT 514
USA: 8645, 8645 to ASTM A29/A29M, 8645 to ASTM A322-91, 8645 to ASTM A331-95, 8645 to ASTM A519, 8645 to ASTM A752/A752M, 8645 to DoD-F-24669/1, 8645 to MIL-S-16974E, 8645 to SAE J404, 8645 to SAE J770, 8645H, 8645H to ASTM A304, 8645H to ASTM A331-95, 8645H to SAE J1268, 8647, 86B45, 86B45 to ASTM A519, 86B45H, 86B45H to ASTM A304, 86B45H to ASTM A331-95, 86B45H to SAE J1268, 8745, G86450 to ASTM A1031, G86450 to SAE J775, NV5 to SAE J775, UNS G86450, UNS G86451, UNS H86450, UNS H86451