AISI 86B45 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 86B45 Oil Quenched & Tempered at 425°C Material Data Sheet

AISI 86B45 Oil Quenched & Tempered at 425°C Overview

AISI 86B45 tempered 425°C is AISI 86B45 low alloy steel (UNS G86451) in the oil quenched & tempered at 425°C condition. This AISI 86B45 tempered 425°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 86B45 conditions in our AISI 86B45 yield, tensile and hardness comparison. Looking for AISI 86B45 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 86B45 steel parts in-house and inspects them before shipment.

AISI 86B45 Oil Quenched & Tempered at 425°C Designation

AISI 86B45
ConditionTempered at 425°C & oil quenched
UNS numberG86451

AISI 86B45 Oil Quenched & Tempered at 425°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 86B45 Oil Quenched & Tempered at 425°C Composition detail

B (boron)5e-4–0.003%
C (carbon)0.43–0.48%
Cr (chromium)0.4–0.6%
Fe (iron)96.5–97.7%
Mn (manganese)0.75–1%
Mo (molybdenum)0.15–0.25%
Ni (nickel)0.4–0.7%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 86B45 Oil Quenched & Tempered at 425°C Physical properties

Density7.8–7.9g/cm3

AISI 86B45 Oil Quenched & Tempered at 425°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)1190–1450MPa
Tensile strength1240–1520MPa
Specific strength151–185kN.m/kg
Elongation8.5–13.5% strain
Compressive strength1190–1450MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)1190–1450MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor18
Hardness – Vickers355–438HV
Elastic stored energy (springs)3430–5050kJ/m3
Fatigue strength at 10^7 cycles497–574MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
435–657MPa

AISI 86B45 Oil Quenched & Tempered at 425°C Impact & fracture properties

Fracture toughness30–55MPa.m0.5
Toughness (G)4.68–13.7kJ/m2

AISI 86B45 Oil Quenched & Tempered at 425°C Thermal properties

Melting point1420–1500°C
Maximum service temperature385–415°C
Minimum service temperature-58–-33°C
Thermal conductivity35–46W/m.°C
Specific heat capacity460–500J/kg.°C
Thermal expansion coefficient11–12.5µstrain/°C
Thermal shock resistance480–611°C
Thermal distortion resistance2.95–3.97MW/m
Latent heat of fusion265–280kJ/kg

AISI 86B45 Oil Quenched & Tempered at 425°C Electrical properties

Electrical resistivity23–35µohm.cm
Electrical conductivity4.93–7.5%IACS
Galvanic potential-0.5–-0.42V

AISI 86B45 Oil Quenched & Tempered at 425°C Magnetic properties

Magnetic typeMagnetic

AISI 86B45 Oil Quenched & Tempered at 425°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)2.8e-4–3.5e-4 

AISI 86B45 Oil Quenched & Tempered at 425°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed11.6 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.692 – 0.863

AISI 86B45 Oil Quenched & Tempered at 425°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 86B45 Oil Quenched & Tempered at 425°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 86B45 Oil Quenched & Tempered at 425°C Standards with similar compositions

Australia: 8645 to AS 1444, 8645H to AS 1444
Mexico: 8645 to NMX-B-203-SCFI, 8645 to NMX-B-300, 8645H to NMX-B-268, 8645H to NMX-B-300, 86B45H to NMX-B-268, 86B45H to NMX-B-300
Pan America: 8645 to COPANT 514, 86B45 to COPANT 514
USA: 8645, 8645 to ASTM A29/A29M, 8645 to ASTM A322-91, 8645 to ASTM A331-95, 8645 to ASTM A519, 8645 to ASTM A752/A752M, 8645 to DoD-F-24669/1, 8645 to MIL-S-16974E, 8645 to SAE J404, 8645 to SAE J770, 8645H, 8645H to ASTM A304, 8645H to ASTM A331-95, 8645H to SAE J1268, 8647, 86B45, 86B45 to ASTM A519, 86B45H, 86B45H to ASTM A304, 86B45H to ASTM A331-95, 86B45H to SAE J1268, 8745, G86450 to ASTM A1031, G86450 to SAE J775, NV5 to SAE J775, UNS G86450, UNS G86451, UNS H86450, UNS H86451