AISI 8620 Normalized Material Data Sheet
AISI 8620 Normalized Overview
| AISI 8620 normalized is AISI 8620 low alloy steel (UNS G86200, EN 20NiCrMo2-2) in the normalized condition. This AISI 8620 normalized material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 8620 conditions in our AISI 8620 yield, tensile and hardness comparison. Looking for AISI 8620 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 8620 steel parts in-house and inspects them before shipment. |
AISI 8620 Normalized Designation
| AISI 8620 | |
| Condition | Normalized |
| UNS number | G86200 |
| US name | SAE 8720H, SAE 8720, SAE 8620, ASTM H86200, ASTM 8620, ASTM G87200, ASTM G86200, ASTM 8720H, ASTM 8720, ASTM 8620H, ASTM 8620, ~ASTM G86170, ~AMS 6277, ~AMS 6276 |
| EN name | 20NiCrMoS2-2, 20NiCrMo2-2 |
| ISO name | Type 20 NiCrMo 2, 20NiCrMo2E |
| GB (Chinese) name | 20CrNiMoH |
| JIS (Japanese) name | SNCM220RCH, SNCM220M, SNCM220H, SNCM220 |
AISI 8620 Normalized Typical uses
| Transmission components in a wide variety of vehicles, general machine parts requiring a hard wear resistant case |
AISI 8620 Normalized Composition detail
| C (carbon) | 0.18 | – | 0.23 | % |
| Cr (chromium) | 0.4 | – | 0.6 | % |
| Fe (iron) | 96.9 | – | 98 | % |
| Mn (manganese) | 0.7 | – | 0.9 | % |
| Mo (molybdenum) | 0.15 | – | 0.25 | % |
| Ni (nickel) | 0.4 | – | 0.7 | % |
| P (phosphorus) | 0 | – | 0.035 | % |
| S (sulfur) | 0 | – | 0.04 | % |
| Si (silicon) | 0.15 | – | 0.35 | % |
AISI 8620 Normalized Physical properties
| Density | 7.8 | – | 7.9 | g/cm3 |
AISI 8620 Normalized Mechanical properties
| Young’s modulus | 201 | – | 212 | GPa |
| Specific stiffness | 25.6 | – | 27 | MN.m/kg |
| Yield strength (elastic limit) | 320 | – | 400 | MPa |
| Tensile strength | 570 | – | 700 | MPa |
| Specific strength | 40.8 | – | 51 | kN.m/kg |
| Elongation | 20 | – | 32 | % strain |
| Compressive strength | 320 | – | 400 | MPa |
| Flexural modulus | 201 | – | 212 | GPa |
| Flexural strength (modulus of rupture) | 320 | – | 400 | MPa |
| Shear modulus | 77 | – | 83 | GPa |
| Bulk modulus | 155 | – | 173 | GPa |
| Poisson’s ratio | 0.285 | – | 0.295 | |
| Shape factor | 57 | |||
| Hardness – Vickers | 170 | – | 210 | HV |
| Elastic stored energy (springs) | 251 | – | 384 | kJ/m3 |
| Fatigue strength at 10^7 cycles | 288 | – | 334 | MPa |
| Fatigue strength model (stress range) Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles | 250 | – | 385 | MPa |
AISI 8620 Normalized Impact & fracture properties
| Fracture toughness | 86 | – | 137 | MPa.m0.5 |
| Toughness (G) | 37.4 | – | 87 | kJ/m2 |
AISI 8620 Normalized Thermal properties
| Melting point | 1480 | – | 1520 | °C |
| Maximum service temperature | 638 | – | 660 | °C |
| Minimum service temperature | -73 | – | -48 | °C |
| Thermal conductivity | 37 | – | 49 | W/m.°C |
| Specific heat capacity | 460 | – | 500 | J/kg.°C |
| Thermal expansion coefficient | 11 | – | 13 | µstrain/°C |
| Thermal shock resistance | 126 | – | 167 | °C |
| Thermal distortion resistance | 3.03 | – | 4.18 | MW/m |
| Latent heat of fusion | 265 | – | 280 | kJ/kg |
AISI 8620 Normalized Electrical properties
| Electrical resistivity | 23 | – | 35 | µohm.cm |
| Electrical conductivity | 4.93 | – | 7.5 | %IACS |
| Galvanic potential | -0.51 | – | -0.43 | V |
AISI 8620 Normalized Magnetic properties
| Magnetic type | Magnetic |
AISI 8620 Normalized Optical, aesthetic and acoustic properties
| Transparency | Opaque | |||
| Acoustic velocity | 5060 | – | 5200 | m/s |
| Mechanical loss coefficient (tan delta) | 7.9e-4 | – | 9.9e-4 | |
AISI 8620 Normalized Processing properties
| Metal casting | Unsuitable |
| Metal cold forming | Excellent |
| Metal hot forming | Excellent |
| Metal press forming | Excellent |
| Metal deep drawing | Limited use |
| Machining speed | 26.5 m/min |
| Weldability Notes: Preheating and post weld heat treatments are required | Good |
| Carbon equivalency | 0.433 – 0.597 |
AISI 8620 Normalized Durability
| Water (fresh) | Acceptable |
| Water (salt) | Limited use |
| Weak acids | Limited use |
| Strong acids | Unacceptable |
| Weak alkalis | Acceptable |
| Strong alkalis | Limited use |
| Organic solvents | Excellent |
| Oxidation at 500C | Acceptable |
| UV radiation (sunlight) | Excellent |
| Galling resistance (adhesive wear) | Acceptable |
| Flammability | Non-flammable |
AISI 8620 Normalized Corrosion resistance
| Stress corrosion cracking Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments | Slightly susceptible |
AISI 8620 Normalized Notes
| AISI 8620 Normalized Other notes |
| One of the most popular low alloy carburizing grades. |
AISI 8620 Normalized Standards with similar compositions
| Argentina: IRAM 8620 to IAS |
| Australia: 8617 to AS 1444, 8617H to AS 1444, 8620 to AS 1444, 8620H to AS 1444 |
| Belgium: 20NiCrMo2 to NBN 253-03 |
| China: 20CrNiMoH to GB/T 5216 |
| Finland: 21NiCrMo2 to SFS 506, 21NiCrMo2(506) to SFS 506 |
| France: 19NCDB2 to AFNOR NF A35-551, 19NCDB2 to AFNOR NF A35-552, 20NCD2 to AFNOR NF A35-551, 20NCD2 to AFNOR NF A35-553, 22NCD2 to AFNOR NF A35-556, 22NCD2 to AFNOR NF A35-566, 23NCDB2 to AFNOR NF A35-556, 23NCDB4 to AFNOR |
| Germany: 1.6523 to DIN 1652, 1.6523 to DIN 1654, 1.6526 to DIN 1652, 20NiCrMo2-2 to DIN 1652, 21NiCrMo22 to DIN, 21NiCrMoS2 to DIN 1652 |
| India: 20N55Cr50Mo20 to IS 1570, 20Ni2Cr2Mo2 to IS 11952, 20Ni2Cr2Mo2 to IS 1570/4, 20NiCrMo2 to IS 11169/1, 20NiCrMo2 to IS 9175/32 |
| International: 20NiCrMo2 to ISO 683-11, 20NiCrMo2 to ISO 683-18, 20NiCrMo2E to ISO 4954, 20NiCrMoS2 to ISO 683-11, 20NiCrMoS2 to ISO 683-18 |
| Italy: 20NiCrMo2 to UNI 7846, 20NiCrMo2 to UNI 8550, 20NiCrMo2 to UNI 8788 |
| Japan: SNCM21 to JIS G4103, SNCM220HRCH to JIS G3509-1, SNCM220RCH to JIS G3509-1 |
| Mexico: 8617 to NMX-B-300, 8620 to NMX-B-203-SCFI, 8620 to NMX-B-300, 8620H to NMX-B-268, 8620H to NMX-B-300, 8622 to NMX-B-203-SCFI, 8622 to NMX-B-300, 8622H to NMX-B-268, 8622H to NMX-B-300, 8720 to NMX-B-300, 8720H to NMX-B-268, 8720H to NMX-B-300 |
| Pan America: 8617 to COPANT 334, 8720 to COPANT 334 |
| Poland: 20HNM to PN-H-84030/02, 22HNM to PN-H-84030/02 |
| Russia: 20KHGNM to GOST 4543 |
| South Korea: SNCM 220 H to KS D 3754 |
| Spain: 20NiCrMo2 to UNE 36013, 20NiCrMo2-1 to UNE 36013, F.1522 to UNE 36013, F.1532 to UNE 36013 |
| Sweden: 2506 to SS 142506 |
| UK: 20NiCrMo2-2 to BS EN 10084, 20NiCrMo2-2 to BS EN 10297-1, 20NiCrMoS2-2 to BS EN 10084, 20NiCrMoS2-2 to BS EN 10277-4, 20NiCrMoS2-2 to BS EN 10297-1, 805A17 to BS 970/1, 805A20 to BS 970/1, 805H20 to BS 970/3, 805H22 to BS 970/3, 805M17 to BS 970/1, 805M20 to BS 970/1, 805M22 to BS 970/1, 806M20 to BS 2772-2, 806M22 to BS 2772-2 |
| USA: 6272 to AMS 6272, 8617, 8617 to ASTM A29/A29M, 8617 to ASTM A331-95, 8617 to ASTM A519, 8617 to ASTM A829/A829M, 8617 to SAE J404, 8617 to SAE J770, 8620, 8620 to ASTM A29/A29M, 8620 to ASTM A331-95, 8620 to ASTM A513, 8620 to ASTM A519, 8620 to ASTM A829/A829M, 8620 to DoD-F-24669/1, 8620 to FED QQ-S-626C, 8620 to MIL-S-16974E, 8620 to SAE J404, 8620 to SAE J770, 8620H to SAE J1975, 8622, 8622 to ASTM A29/A29M, 8622 to ASTM A331-95, 8622 to ASTM A519, 8622 to ASTM A829/A829M, 8622 to DoD-F-24669/1, 8622 to SAE J404, 8622 to SAE J770, 8717, 8719, 8720 to ASTM A29/A29M, 8720 to ASTM A331-95, 8720 to ASTM A519, 8720 to SAE J404, 8720 to SAE J770, 8720H to SAE J1975, EX 5, G86170 to ASTM A1031, G86200 to ASTM A1031, G86200 to ASTM A507, G87200 to ASTM A1031, Grade 4 to ASTM A646-95, H86200 to ASTM A506, UNS G86170, UNS G86200, UNS G86220, UNS G87200, UNS H86170, UNS H86200, UNS H86220, UNS H87200, UNS K11948, UNS K12147 |
| Tradenames: 20 NI CR MO 2, A-1522, ACENOR F-1522, AFORA 19 NCDB2, ASCOMETAL 20NCD2, FORTUNA EX8H, KRUPP 21 NICRMO 2 2, KRUPP 21 NICRMOS 2, LASALLE 8620, OVAKO 152, POMPEY B 8620, SAARSTAHL 21 NICRMO 2, SHARON 8600 SERIES A, TKS 21 NICRMO 2, VB-20, VERTOMAR CNM20 |