AISI 51B60 Oil Quenched & Tempered at 650°C Material Data Sheet

AISI 51B60 Oil Quenched & Tempered at 650°C Material Data Sheet

AISI 51B60 Oil Quenched & Tempered at 650°C Overview

AISI 51B60 tempered 650°C is AISI 51B60 low alloy steel (UNS G51601) in the oil quenched & tempered at 650°C condition. This AISI 51B60 tempered 650°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 51B60 conditions in our AISI 51B60 yield, tensile and hardness comparison. Looking for AISI 51B60 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 51B60 steel parts in-house and inspects them before shipment.

AISI 51B60 Oil Quenched & Tempered at 650°C Designation

AISI 51B60
ConditionTempered at 650°C & oil quenched
UNS numberG51601
US nameASTM 51B60, ~ASTM 50B60, ~ASTM 51B60

AISI 51B60 Oil Quenched & Tempered at 650°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 51B60 Oil Quenched & Tempered at 650°C Composition detail

B (boron)5e-4–0.003%
C (carbon)0.56–0.64%
Cr (chromium)0.7–0.9%
Fe (iron)97–97.8%
Mn (manganese)0.75–1%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 51B60 Oil Quenched & Tempered at 650°C Physical properties

Density7.8–7.9g/cm3

AISI 51B60 Oil Quenched & Tempered at 650°C Mechanical properties

Young’s modulus201–212GPa
Specific stiffness25.6–27MN.m/kg
Yield strength (elastic limit)780–960MPa
Tensile strength865–1070MPa
Specific strength99.3–122kN.m/kg
Elongation16–24% strain
Compressive strength780–960MPa
Flexural modulus201–212GPa
Flexural strength (modulus of rupture)780–960MPa
Shear modulus77–83GPa
Bulk modulus155–173GPa
Poisson’s ratio0.285–0.295 
Shape factor28
Hardness – Vickers265–325HV
Elastic stored energy (springs)1490–2210kJ/m3
Fatigue strength at 10^7 cycles386–448MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
336–515MPa

AISI 51B60 Oil Quenched & Tempered at 650°C Impact & fracture properties

Fracture toughness42–71MPa.m0.5
Toughness (G)9.02–23.1kJ/m2

AISI 51B60 Oil Quenched & Tempered at 650°C Thermal properties

Melting point1380–1490°C
Maximum service temperature587–640°C
Minimum service temperature-68–-38°C
Thermal conductivity41–48W/m.°C
Specific heat capacity440–520J/kg.°C
Thermal expansion coefficient11.5–13µstrain/°C
Thermal shock resistance304–387°C
Thermal distortion resistance3.29–4MW/m
Latent heat of fusion265–280kJ/kg

AISI 51B60 Oil Quenched & Tempered at 650°C Electrical properties

Electrical resistivity22–30µohm.cm
Electrical conductivity5.75–7.84%IACS
Galvanic potential-0.5–-0.42V

AISI 51B60 Oil Quenched & Tempered at 650°C Magnetic properties

Magnetic typeMagnetic

AISI 51B60 Oil Quenched & Tempered at 650°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5200m/s
Mechanical loss coefficient (tan delta)4.1e-4–5.2e-4 

AISI 51B60 Oil Quenched & Tempered at 650°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed16.8 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Poor
Carbon equivalency0.825 – 0.987

AISI 51B60 Oil Quenched & Tempered at 650°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 51B60 Oil Quenched & Tempered at 650°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Slightly susceptible

AISI 51B60 Oil Quenched & Tempered at 650°C Standards with similar compositions

China: 60CrMnBA to GB 1222
Pan America: 51B60 to COPANT 514
USA: 51B60, 51B60 to ASTM A29/A29M, 51B60 to ASTM A322-91, 51B60 to SAE J770, 51B60H, 51B60H to ASTM A304, 51B60H to SAE J1268, UNS H51601