AISI 5130 Oil Quenched & Tempered at 205°C Material Data Sheet

AISI 5130 Oil Quenched & Tempered at 205°C Material Data Sheet

AISI 5130 Oil Quenched & Tempered at 205°C Overview

AISI 5130 tempered 205°C is AISI 5130 low alloy steel (UNS G51300, EN 34Cr4) in the oil quenched & tempered at 205°C condition. This AISI 5130 tempered 205°C material data sheet covers its designation, chemical composition, physical, mechanical, thermal, electrical and magnetic properties, processing and corrosion behaviour, and standards with similar compositions. Compare all AISI 5130 conditions in our AISI 5130 yield, tensile and hardness comparison. Looking for AISI 5130 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 5130 steel parts in-house and inspects them before shipment.

AISI 5130 Oil Quenched & Tempered at 205°C Designation

AISI 5130
ConditionTempered at 205°C & oil quenched
UNS numberG51300
US nameSAE 5130, SAE 5132H, SAE 5132, ASTM 5130, ASTM G51300, ASTM 5132H, ASTM 5132, ASTM 5130H, ASTM 5130, ~ASTM 5130
EN name~34CrS4, ~34Cr4, ~28Cr4
EN number~1.7037, ~1.7033, ~1.703
ISO name34CrS4, 34Cr4, 1b, ~34Cr4
GB (Chinese) name~30CrMnSiA

AISI 5130 Oil Quenched & Tempered at 205°C Typical uses

General construction, general mechanical engineering, automotive, tools, axles, gears, springs.

AISI 5130 Oil Quenched & Tempered at 205°C Composition detail

C (carbon)0.28–0.33%
Cr (chromium)0.8–1.1%
Fe (iron)97.2–98.1%
Mn (manganese)0.7–0.9%
P (phosphorus)0–0.035%
S (sulfur)0–0.04%
Si (silicon)0.15–0.35%

AISI 5130 Oil Quenched & Tempered at 205°C Physical properties

Density7.8–7.9g/cm3

AISI 5130 Oil Quenched & Tempered at 205°C Mechanical properties

Young’s modulus201–217GPa
Specific stiffness25.6–27.7MN.m/kg
Yield strength (elastic limit)1370–1670MPa
Tensile strength1460–1780MPa
Specific strength174–213kN.m/kg
Elongation8–12% strain
Compressive strength1370–1670MPa
Flexural modulus201–217GPa
Flexural strength (modulus of rupture)1370–1670MPa
Shear modulus77–85GPa
Bulk modulus155–177GPa
Poisson’s ratio0.285–0.295 
Shape factor15
Hardness – Vickers425–525HV
Elastic stored energy (springs)4490–6630kJ/m3
Fatigue strength at 10^7 cycles556–641MPa
Fatigue strength model (stress range)
Parameters: Stress Ratio = -1, Number of Cycles = 1e7cycles
487–732MPa

AISI 5130 Oil Quenched & Tempered at 205°C Impact & fracture properties

Fracture toughness27–50MPa.m0.5
Toughness (G)3.75–11.1kJ/m2

AISI 5130 Oil Quenched & Tempered at 205°C Thermal properties

Melting point1460–1510°C
Maximum service temperature165–195°C
Minimum service temperature-53–-28°C
Thermal conductivity45–50W/m.°C
Specific heat capacity470–530J/kg.°C
Thermal expansion coefficient11.5–13µstrain/°C
Thermal shock resistance523–668°C
Thermal distortion resistance3.58–4.2MW/m
Latent heat of fusion265–280kJ/kg

AISI 5130 Oil Quenched & Tempered at 205°C Electrical properties

Electrical resistivity18–24µohm.cm
Electrical conductivity7.18–9.58%IACS
Galvanic potential-0.5–-0.42V

AISI 5130 Oil Quenched & Tempered at 205°C Magnetic properties

Magnetic typeMagnetic

AISI 5130 Oil Quenched & Tempered at 205°C Optical, aesthetic and acoustic properties

TransparencyOpaque
Acoustic velocity5060–5260m/s
Mechanical loss coefficient (tan delta)2.4e-4–3e-4 

AISI 5130 Oil Quenched & Tempered at 205°C Processing properties

Metal castingUnsuitable
Metal cold formingExcellent
Metal hot formingExcellent
Metal press formingExcellent
Metal deep drawingLimited use
Machining speed10.1 m/min
Weldability
Notes: Preheating and post weld heat treatments are required
Good
Carbon equivalency0.557 – 0.7

AISI 5130 Oil Quenched & Tempered at 205°C Durability

Water (fresh)Acceptable
Water (salt)Limited use
Weak acidsLimited use
Strong acidsUnacceptable
Weak alkalisAcceptable
Strong alkalisLimited use
Organic solventsExcellent
Oxidation at 500CAcceptable
UV radiation (sunlight)Excellent
Galling resistance (adhesive wear)Acceptable
FlammabilityNon-flammable

AISI 5130 Oil Quenched & Tempered at 205°C Corrosion resistance

Stress corrosion cracking
Note: Rated in chloride; May be susceptible in halide, ammonia, nitrogen, acidic, caustic, carbonate environments
Susceptible

AISI 5130 Oil Quenched & Tempered at 205°C Standards with similar compositions

Argentina: IRAM 5130 to IAS, IRAM 5132 to IAS
Australia: 5132 to AS 1444, 5132H to AS 1444
Belgium: 34Cr4 to NBN 251
China: 30Cr to GB/T 11251
France: 32C4 to AFNOR NF A35-552, 32C4 to AFNOR NF A35-553, 32C4 to AFNOR NF A35-556, 32C4 to AFNOR NF A35-557
Germany: 1.7030 to DIN EN 10083, 1.7033 to DIN 1652, 1.7033 to DIN EN 10083, 1.7037 to DIN EN 10083, 28Cr4 to DIN EN 10083, 34Cr4 to DIN 1652, 34Cr4 to DIN EN 10083, 34CrS4 to DIN EN 10083
Hungary: Cr1 to MSZ 61, Cr1E to MSZ 61, Cr1Z to MSZ 6251
International: 1 to ISO 683-7, 1a to ISO 683-7, 1b to ISO 683-7, 34Cr4 to ISO 683-1, 34Cr4 to ISO 683-18, 34Cr4E to ISO 4954, 34CrS4 to ISO 683-1, 34CrS4 to ISO 683-18
Italy: 34Cr4 to UNI 7874, 34Cr4KB to UNI 7356
Japan: SCr2H to JIS G4052, SCr3H to JIS G4052, SCr430HRCH to JIS G3509-1, SCr430RCH to JIS G3509-1
Mexico: 5130 to NMX-B-203-SCFI, 5130 to NMX-B-300, 5130H to NMX-B-268, 5130H to NMX-B-300, 5132 to NMX-B-203-SCFI, 5132 to NMX-B-300, 5132H to NMX-B-268, 5132H to NMX-B-300, 5135 to NMX-B-300, 5135H to NMX-B-268, 5135H to NMX-B-300
Pan America: 5130 to COPANT 334, 5135 to COPANT 334
Romania: 32Cr10 to STAS 11500/2
South Korea: SCr 430 H to KS D 3754, SCr 430 to KS D 3707, SCr 435 H to KS D 3754, SCr 435 to KS D 3707
UK: 28Cr4 to BS EN 10084, 28CrS4 to BS EN 10084, 34Cr4 to BS EN 10083-1, 34Cr4 to BS EN 10250-3, 34CrS4 to BS EN 10083-1, 34CrS4 to BS EN 10277-5
USA: 5130 to ASTM A29/A29M, 5130 to ASTM A331-95, 5130 to ASTM A513, 5130 to ASTM A519, 5130 to SAE J404, 5132 to ASTM A29/A29M, 5132 to ASTM A331-95, 5132 to ASTM A519, 5132 to SAE J404, 5132 to SAE J770, 5135, 5135 to ASTM A29/A29M, 5135 to ASTM A331-95, 5135 to ASTM A519, G51300 to ASTM A1031, G51320 to ASTM A1031, UNS G51300, UNS G51320, UNS G51350, UNS H51300, UNS H51320, UNS H51350
Tradenames: 34 CR 4, AMBO VC 135, ASCOMETAL 32C4, BOHLER KMC, CREUSOT 1F4/5, CREUSOT 1F5/6, FORTUNA TC4, KRUPP 28 CR 4, KRUPP 28 CRS 4, KRUPP 32 CRB 4, KRUPP 34 CRS 4, POMPEY DK 35, SAARSTAHL 34 CR 4, SCHNEIDER 1F 3/4, SCHNEIDER 1F 4/5, STEEL 34 CR 4, SUWEFA TC4, TKS 34CR4, VR-30