AISI 94B30 Tempering Temperature Comparison (205–650°C): Yield, Tensile & Hardness

How do the AISI 94B30 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 94B30 (UNS G94301) side by side for 5 conditions: Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 94B30 material data sheets linked below.

AISI 94B30 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 205°C1400–17101550–1900425–5259–15
Oil Quenched & Tempered at 315°C1280–15701440–1760400–4909–15
Oil Quenched & Tempered at 425°C1090–13301210–1480345–42510–16
Oil Quenched & Tempered at 540°C835–1030900–1100275–34513–19
Oil Quenched & Tempered at 650°C650–795740–915228–28316–26

AISI 94B30 Differences Compared with Oil Quenched & Tempered at 205°C

The table below shows how much each condition differs from the oil quenched & tempered at 205°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 315°C-8%-7%-6%+0%
Oil Quenched & Tempered at 425°C-22%-22%-19%+8%
Oil Quenched & Tempered at 540°C-40%-42%-35%+33%
Oil Quenched & Tempered at 650°C-54%-52%-46%+75%

AISI 94B30 Strength and Hardness Charts

AISI 94B30 Yield strength (MPa)Q&T 205°C1400–1710Q&T 315°C1280–1570Q&T 425°C1090–1330Q&T 540°C835–1030Q&T 650°C650–795
AISI 94B30 Tensile strength (MPa)Q&T 205°C1550–1900Q&T 315°C1440–1760Q&T 425°C1210–1480Q&T 540°C900–1100Q&T 650°C740–915
AISI 94B30 Hardness (HV)Q&T 205°C425–525Q&T 315°C400–490Q&T 425°C345–425Q&T 540°C275–345Q&T 650°C228–283

AISI 94B30 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1550–1900 MPa). The softest condition is oil quenched & tempered at 650°C (228–283 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 425–525 HV to 228–283 HV, trading strength for toughness and ductility.

AISI 94B30 Material Data Sheets

AISI 94B30 Oil Quenched & Tempered at 205°C | AISI 94B30 Oil Quenched & Tempered at 315°C | AISI 94B30 Oil Quenched & Tempered at 425°C | AISI 94B30 Oil Quenched & Tempered at 540°C | AISI 94B30 Oil Quenched & Tempered at 650°C | All AISI 94B30 conditions