AISI 9260 Tempering Temperature Comparison (425–650°C): Yield, Tensile & Hardness

How do the AISI 9260 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 9260 (UNS G92600, EN 60Si7) side by side for 3 conditions: Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 9260 material data sheets linked below.

AISI 9260 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 425°C1350–16601580–1940420–5206–10
Oil Quenched & Tempered at 540°C1020–12501190–1460353–4339–15
Oil Quenched & Tempered at 650°C730–895880–1080270–33016–24

AISI 9260 Differences Compared with Oil Quenched & Tempered at 425°C

The table below shows how much each condition differs from the oil quenched & tempered at 425°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 540°C-25%-25%-16%+50%
Oil Quenched & Tempered at 650°C-46%-44%-36%+150%

AISI 9260 Strength and Hardness Charts

AISI 9260 Yield strength (MPa)Q&T 425°C1350–1660Q&T 540°C1020–1250Q&T 650°C730–895
AISI 9260 Tensile strength (MPa)Q&T 425°C1580–1940Q&T 540°C1190–1460Q&T 650°C880–1080
AISI 9260 Hardness (HV)Q&T 425°C420–520Q&T 540°C353–433Q&T 650°C270–330

AISI 9260 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 425°C condition (1580–1940 MPa). The softest condition is oil quenched & tempered at 650°C (270–330 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 425°C to 650°C lowers hardness from 420–520 HV to 270–330 HV, trading strength for toughness and ductility.

AISI 9260 Material Data Sheets