AISI 86B45 Tempering Temperature Comparison (205–650°C): Yield, Tensile & Hardness

How do the AISI 86B45 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 86B45 (UNS G86451) side by side for 5 conditions: Oil Quenched & Tempered at 205°C, Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 86B45 material data sheets linked below.

AISI 86B45 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 205°C1490–18101780–2180470–5807–11
Oil Quenched & Tempered at 315°C1400–17101530–1870425–5257–11
Oil Quenched & Tempered at 425°C1190–14501240–1520355–4388.5–13.5
Oil Quenched & Tempered at 540°C925–1140990–1220303–37312–18
Oil Quenched & Tempered at 650°C785–970810–995255–31515–23

AISI 86B45 Differences Compared with Oil Quenched & Tempered at 205°C

The table below shows how much each condition differs from the oil quenched & tempered at 205°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 315°C-6%-14%-10%+0%
Oil Quenched & Tempered at 425°C-20%-30%-24%+22%
Oil Quenched & Tempered at 540°C-37%-44%-36%+67%
Oil Quenched & Tempered at 650°C-47%-54%-46%+111%

AISI 86B45 Strength and Hardness Charts

AISI 86B45 Yield strength (MPa)Q&T 205°C1490–1810Q&T 315°C1400–1710Q&T 425°C1190–1450Q&T 540°C925–1140Q&T 650°C785–970
AISI 86B45 Tensile strength (MPa)Q&T 205°C1780–2180Q&T 315°C1530–1870Q&T 425°C1240–1520Q&T 540°C990–1220Q&T 650°C810–995
AISI 86B45 Hardness (HV)Q&T 205°C470–580Q&T 315°C425–525Q&T 425°C355–438Q&T 540°C303–373Q&T 650°C255–315

AISI 86B45 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 205°C condition (1780–2180 MPa). The softest condition is oil quenched & tempered at 650°C (255–315 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 205°C to 650°C lowers hardness from 470–580 HV to 255–315 HV, trading strength for toughness and ductility.

AISI 86B45 Material Data Sheets

AISI 86B45 Oil Quenched & Tempered at 205°C | AISI 86B45 Oil Quenched & Tempered at 315°C | AISI 86B45 Oil Quenched & Tempered at 425°C | AISI 86B45 Oil Quenched & Tempered at 540°C | AISI 86B45 Oil Quenched & Tempered at 650°C | All AISI 86B45 conditions

Looking for AISI 86B45 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 86B45 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.