AISI 50B46 Tempering Temperature Comparison (315–650°C): Yield, Tensile & Hardness

How do the AISI 50B46 heat treatment properties change from one condition to another? This comparison puts the yield strength, tensile strength and hardness of AISI 50B46 (UNS G50461) side by side for 4 conditions: Oil Quenched & Tempered at 315°C, Oil Quenched & Tempered at 425°C, Oil Quenched & Tempered at 540°C, Oil Quenched & Tempered at 650°C. All values are taken from the individual AISI 50B46 material data sheets linked below.

AISI 50B46 Yield, Tensile and Hardness by Condition

ConditionYield strength (MPa)Tensile strength (MPa)Hardness (HV)Elongation (%)
Oil Quenched & Tempered at 315°C1460–17801600–1960455–5558–12
Oil Quenched & Tempered at 425°C1120–13801250–1540365–44510–16
Oil Quenched & Tempered at 540°C880–1080970–1200290–36013–21
Oil Quenched & Tempered at 650°C710–875800–965250–30517–27

AISI 50B46 Differences Compared with Oil Quenched & Tempered at 315°C

The table below shows how much each condition differs from the oil quenched & tempered at 315°C condition, based on the mid-point of each range. Positive values mean higher strength or hardness.

ConditionYield strengthTensile strengthHardnessElongation
Oil Quenched & Tempered at 425°C-23%-22%-20%+30%
Oil Quenched & Tempered at 540°C-40%-39%-36%+70%
Oil Quenched & Tempered at 650°C-51%-50%-45%+120%

AISI 50B46 Strength and Hardness Charts

AISI 50B46 Yield strength (MPa)Q&T 315°C1460–1780Q&T 425°C1120–1380Q&T 540°C880–1080Q&T 650°C710–875
AISI 50B46 Tensile strength (MPa)Q&T 315°C1600–1960Q&T 425°C1250–1540Q&T 540°C970–1200Q&T 650°C800–965
AISI 50B46 Hardness (HV)Q&T 315°C455–555Q&T 425°C365–445Q&T 540°C290–360Q&T 650°C250–305

AISI 50B46 Heat Treatment Key Points

The highest tensile strength is reached in the oil quenched & tempered at 315°C condition (1600–1960 MPa). The softest condition is oil quenched & tempered at 650°C (250–305 HV), which is usually preferred for machining and forming. Raising the tempering temperature from 315°C to 650°C lowers hardness from 455–555 HV to 250–305 HV, trading strength for toughness and ductility.

AISI 50B46 Material Data Sheets

AISI 50B46 Oil Quenched & Tempered at 315°C | AISI 50B46 Oil Quenched & Tempered at 425°C | AISI 50B46 Oil Quenched & Tempered at 540°C | AISI 50B46 Oil Quenched & Tempered at 650°C | All AISI 50B46 conditions

Looking for AISI 50B46 parts from Turkey (Türkiye)? Modulus Metal manufactures CNC machined AISI 50B46 steel parts in-house, heat treated to the condition you specify, and inspects them before shipment.